Showerthought: flux or no flux when forge welding my first billet taught me more than any video
Last month I finally tried my first pattern weld and had to pick between borax flux and going fluxless in my little coal forge out back, and I went with borax. The welds stuck on the second heat but the slag cleanup ate about 40 minutes I wasn't planning on. Anyone here run fluxless on a coal fire, or is that just asking for a cold shut every time?
Fluxless on coal is doable but you gotta babysit the fire way more than with gas. Coal throws sulfur and junk into the weld zone, so you have to run it just past the smoke stage and keep the billet in the sweet spot of the fire, not buried in the green coal. The trick is a good scarf and a clean fire, and you really want the two pieces to mate tight before the first hit. I'd say try one small test billet fluxless before you write it off, because losing 40 minutes to slag cleanup on every weld adds up fast. Borax is forgiving though, so no shame in sticking with it while you're learning.